Silicone Compression Set, CFD, Durometer and the Other Properties That Decide a Gasket
Compression force deflection tells you how hard a silicone gasket pushes back on the day it is installed; compression set tells you how much of that is left after heat and time. This page explains both, with the test conditions behind the numbers and a benchmark across silicone foam, sponge, solid, urethane, and EPDM, then works through the other sixteen properties an engineer meets on a silicone data sheet.
Part of the Silicone Materials guide. Start at the hub page for the forms, the selection matrix and the material families; this page goes deep on one topic.
Design cellular silicone at 25–35% deflection and compute closure force as stress at that deflection times gasket footprint. Compare compression set only on the same method, deflection, temperature and time: cast silicone foam sets about 2–5% (ASTM D1056, 100 °C/22 h/50%), blown sponge 15–20%, AMS sponge specs permit 60%, and EPDM sponge runs 35–48% in Rogers’ comparison. Every other property on this page is explained by what to do with it, not just what it is. Skip to the quote form →

Compression force deflection (CFD) is the stress needed to compress a cellular silicone by a stated percentage, usually 25%, per ASTM D1056; it sets closure force. Compression set is the permanent thickness lost after the material is held compressed at temperature (BISCO basis: 50%, 100 °C, 22 h) and released; it predicts whether the gasket is still pressing on the flange in year three. Cast silicone foam sets about 2–5% on that basis, blown sponge 15–20%, and solid silicone is measured separately by ASTM D395 at 25% deflection.
Property values are quoted from the source manufacturer TDS or the cited standard, not from H-O testing. H-O converts sheet and roll silicone; ratings belong to the specific grade and a finished assembly earns its own rating at the system level.
- Closure force: stress at design deflection × footprint area
- Long-term seal: compression set under 5% (D1056, 100 °C)
- Solid vs cellular: D395 at 25% vs D1056 at 50%
-
1Send drawingUpload a DXF, STEP, or PDF, or describe the gasket, pad, or insulator and its environment. A sample part works too.
-
2Material reviewEngineering checks the candidate grade against the manufacturer TDS: closure force, compression set, service temperature, fluid exposure, flame or regulatory requirement, and adhesive compatibility.
-
3Prototype24-hour prototypes on in-house materials; otherwise samples typically ship in 3–5 business days for common die-cut configurations on materials we commonly convert. Made-to-order; MOQ varies by material and part.
-
4ProductionStandard production runs ship about 2 weeks after drawing approval, including kiss-cut-on-liner and laminated configurations. Expedited service available. Ongoing parts run with lot traceability and TDS records.
CFD vs compression set: force today, force in three years
Compression force deflection tells you how hard the gasket pushes back on the day it is installed. Compression set tells you how much of that push-back is gone after heat and time. Engineers routinely specify the first and forget the second, and the result is an enclosure that passes the factory water test and fails the field audit. The two properties come from different tests, use different formulas, and vary between silicone forms by an order of magnitude.
The test conditions behind the numbers
Compression-set values cannot be compared across methods. The three you will meet on silicone and competing materials:
| Method | Applies to | Deflection | Typical condition | Formula | Practical note |
|---|---|---|---|---|---|
| ASTM D1056 Test D | Sponge, cast silicone foam (BISCO) | 50% | 22 h at 70 °C or 100 °C; 30 min recovery | (t₀ − t₁) ÷ (t₀ − spacer) × 100 | Divides by the amount deflected, so numbers read about twice as high as the D3574 formula for the same recovery. [9] |
| ASTM D3574 Test D | Flexible urethane foam (PORON®) | 50% | 22 h at 70 °C | (t₀ − t₁) ÷ t₀ × 100 | A 2% D1056 result ≈ 1% D3574; a PORON “10%” and a BISCO “10%” are not the same recovery. [58] |
| ASTM D395 Method B | Solid rubber | 25% | 22 h or 70 h at 70 °C, 100 °C, 150 °C, or 175 °C | (t₀ − t₁) ÷ (t₀ − spacer) × 100 | BISCO HT-1200 solids: ≤25% at 150 °C/70 h; kSil GP50: 16% at 22 h/300 °F (149 °C). Temperature and time must be stated. [17] [18] |
Benchmark: compression set by material and condition
Values are typical or maximum figures from the cited data sheets and guides on the stated basis; they are for ranking, not for substitution. Where the same material appears at two temperatures, note how quickly the hydrocarbon rubbers separate from silicone as temperature rises.
| Material | Form | Basis | Compression set | Source |
|---|---|---|---|---|
| BISCO® BF-1000 | Cast silicone foam | D1056, 100 °C/22 h/50% | 1.7% typ. | [51] |
| BISCO® HT-800 | Cast silicone foam | D1056, 100 °C/22 h/50% | 2.4% typ. (<5% spec) | [4] |
| BISCO® HT-840 | Cast silicone foam | D1056, 100 °C/22 h/50% | 1.8% typ. (<5% spec) | [59] |
| Norseal® R10460 | Closed-cell silicone sponge | D1056 | 5% | [23] |
| expanSil™ GP400 | Closed-cell silicone sponge (extrusion grade) | Per TDS, 70 °C/22 h and 100 °C/22 h | 3.0% / 4.3% | [60] |
| BISCO® RS-700 series | Blown silicone sponge | D1056, 100 °C/22 h | 15–20% max | [10] |
| BISCO® 7304 Medium | Blown silicone sponge (BMS 1-23) | 22 h at 212 °F | 20% | [68] |
| BISCO® 7130 / 7330 / 7430 FR | Blown silicone sponge (BMS 1-60) | 22 h at 212 °F | 35% | [68] |
| Norseal® R10490 | Fluorosilicone sponge | D1056 | 25% | [61] |
| AMS 3195 / 3196 requirement | Closed-cell silicone sponge (spec limit) | 22 h at 100 °C | 60% max | [19] |
| BISCO® HT-1200 series | Solid silicone, 40–70 A | D395 B, 150 °C/70 h/25% | ≤25% | [17] |
| kSil® GP50 / GP70 | Solid silicone, 50 / 70 A | D395 B, 22 h/300 °F | 16% / 10% | [18] |
| BISCO® EC-2130 | Ni-graphite conductive solid, 30 A | D395 B, 70 °C/70 h/25% | 10% max | [35] |
| PORON® 4701-50 | Cellular urethane | D3574, 70 °C/22 h/50% | ≤10% | [62] |
| EPDM sponge (Rogers guide comparison) | Closed-cell EPDM | 50% / 22 h at 70 °C and 100 °C (method not stated; read from chart) | ≈20–35% / ≈48% | [5] |
| Neoprene/EPDM blend sponge (Rogers guide) | Closed-cell blend | 50% / 22 h at 70 °C (method not stated; read from chart) | ≈25% | [5] |
Worked example: sizing an enclosure gasket
A sheet-metal control-cabinet door, 24 × 36 in, with a 0.5 in wide perimeter gasket has a footprint of about 120 in² (perimeter 120 in × 0.5 in). If the design deflection is 30% and the chosen foam shows 6 psi at 30% on its curve, the latches must supply roughly 720 lb in total, or about 180 lb per latch on a four-latch door. A firm sponge at 15 psi would need 1,800 lb and the door would bow between latches. This is the calculation the CFD calculator and the gasket compression and thickness finder automate. Then check recovery: at 2–5% set the foam gasket retains almost all of its 30% deflection over life; at 20% set (blown sponge) roughly a fifth of the working deflection is consumed by the material, and the tolerance stack must absorb the rest.
Design cellular silicone at 25–35% deflection (Rogers recommends this minimum to absorb thickness tolerance, surface variation, and stress relaxation; 50–70% is permissible but may crush cells). Keep gasket width at least equal to thickness, preferably 1.5×. Design solid silicone at 10–30% deflection, and for water at the upper end. Treat a gap tolerance of about ±2 mm as the practical limit for a 10 mm foam gasket. Under 5% compression set on the D1056 basis is the target for permanently compressed silicone seals; state the basis on the drawing. [14] [48] [16]
Engineering properties of silicone and what to do with them
A data sheet lists properties; a design uses them. Each entry below states what the property is, how it is measured, how an engineer should use it in a silicone part decision, and how much it varies between grades. Expand the ones relevant to your job.
Show all 18 engineering properties tap to collapse
Compression force deflection (CFD)
What it is. The stress (psi or kPa) needed to compress a cellular material by a stated percentage of its thickness, usually 25%. It is the firmness rating of sponge and foam and the input to closure-force calculations.
Measured by. ASTM D1056 (sponge, cast silicone foam) at 25%; ASTM D3574 Test C for urethane foams. Rogers publishes force-vs-deflection data across the deflection range for BISCO grades. [14]
How to use it. Closure force = CFD at your design deflection × gasket footprint area. Rogers’ worked example: 5 psi × 72 in² = 360 lb to reach 25% deflection. Choose the softest grade that still develops the sealing pressure and recovers, and check that the flange and fasteners can supply the force. [48] Use the CFD calculator.
Grade dependency. Very high: under 2 psi to over 20 psi within one foam family. Spec ranges are wide (HT-800: 6–14 psi), so design to the range, not the typical.
Compression set
What it is. The permanent loss of thickness after a material is held compressed at a temperature for a time and then released. It is the single best predictor of whether a gasket will still be pressing on the flange in year three.
Measured by. Cellular: ASTM D1056 (BISCO basis: 50% deflection, 100 °C, 22 h, 30 min recovery; the formula divides by the deflected amount, so a 2% D1056 result is roughly 1% by the D3574 formula). Solid: ASTM D395 Method B (25% deflection; BISCO HT-1200 at 150 °C/70 h). [9] [49]
How to use it. Compare only on the same method, deflection, temperature, and time. Under 5% (D1056, 100 °C) is “excellent for long-term sealing” per Rogers; blown sponge at 15–20% and AMS-permitted 60% are a different tier. Add margin for stress relaxation, which is the loss of force (not thickness) and happens mostly in the first 1–2 hours. [5] See CFD vs compression set.
Grade dependency. Extreme: 2% (cast foam) to 60% (AMS sponge limit) on the same basis.
Durometer (hardness)
What it is. Indentation resistance of a solid elastomer, read on the Shore A scale for rubber sheet and Shore OO for very soft gels and gap pads. It is not stiffness, not compressibility, and not a seal rating.
Measured by. ASTM D2240, on a specimen at least 6 mm thick (thin sheet is plied up). Drawing tolerance is conventionally ±5 points (industry practice; D2240 defines the method, not the tolerance). [50]
How to use it. Pick durometer by how the part is loaded: 20–40 A for conformable, low-force seals and cushioning; 50–60 A for general flange gaskets and washers; 70–90 A where extrusion resistance, dimensional stability, or abrasion matters. Do not use Shore A for sponge or foam; use CFD. The durometer scale chart cross-references the scales.
Grade dependency. Catalog spans 10–90 Shore A (solid) and Shore OO 30–80 (gap pads, sponge reference).
Density and specific gravity
What it is. Mass per volume. For cellular silicone (pcf or kg/m³) it tracks firmness within a family and is the quickest sanity check on a substituted material. For solids, specific gravity reveals filler: unfilled VMQ about 1.1–1.2; ceramic-, metal-, or ferrous-filled grades 1.3–3.6.
Measured by. ASTM D1056 (cellular), ASTM D297 or D792 (solid).
How to use it. Weight budgets in aerospace and EV packs; yield and cost estimates (sheet is often sold by area but shipped by weight); verifying that “equivalent” foam is really equivalent (a 15 pcf and a 22 pcf foam are different grades).
Grade dependency. Foam 5–28 pcf; sponge about 10–37 pcf; solid SG 1.07 (HT-6240) to 3.6 (Gap Pad TGP 5000). [31] [36]
Tensile strength
What it is. Stress at break in a pulled dumbbell specimen. For gaskets it is a proxy for handling toughness and the ability to survive installation, not a service load.
Measured by. ASTM D412 (Die C dumbbell) for solids; also D412 on foams where reported.
How to use it. Screen for assembly robustness and for stretch-fit parts. Foams at 35–60 psi cannot be stretched over a feature; solids at 800–1,300 psi can. Silicone’s tensile (roughly half that of EPDM or neoprene at the same durometer) is why it is not chosen for abrasive or dynamic duty.
Grade dependency. High: 38 psi (BF-1000 foam) to 1,300+ psi (medical and high-tear solids). [51] [11]
Tear strength
What it is. Force per unit thickness (ppi or kN/m) to propagate a tear from a notch. It is the property that decides whether a die-cut gasket survives a bolt hole, a narrow web, or a technician pulling it off a flange.
Measured by. ASTM D624, Die B (most TDS) or Die C; values are not interchangeable between dies.
How to use it. Specify 150+ ppi for parts with bolt holes near edges, thin webs, or repeated removal; add radii to inside corners; consider reinforced sheet for large or thin parts. Fluorosilicone and filled conductive grades often tear more easily than plain VMQ.
Grade dependency. Roughly 75 ppi (commercial 30 A) to 250 ppi (high-tear, medical) in solids; a few ppi in foams.
Elongation at break
What it is. Percent stretch at break (ASTM D412). It indicates conformability, stretch-fit capability, and, when tracked through heat aging, the onset of embrittlement.
How to use it. Membranes and diaphragms need 500–900%; general gaskets need enough to survive assembly (200%+); reinforced sheet has almost none by design. Retained elongation after heat aging (for example, above 90% after 168 h at 300 °C for H-O’s high-temperature sheet) is a better high-temperature metric than any single rating. [7]
Grade dependency. 60% (foam) to 900% (membrane, medical).
Temperature range (continuous, intermittent, low-temperature flexibility)
What it is. Three different numbers that data sheets often blur: the continuous service temperature the manufacturer stands behind for the life of the part; an intermittent or short-term peak; and the low-temperature limit, reported as a brittleness or flex test (ASTM D746, D2137) or a torsional stiffening temperature (Gehman).
How to use it. Design to the continuous rating of the specific grade and confirm that the adhesive, liner, and any reinforcing ply are rated at least as high; a silicone PSA holds to roughly 232 °C while an acrylic PSA holds to roughly 149 °C on Rogers’ bulletin. [26] For cold service, standard VMQ passes flex at −55 °C; phenyl (PVMQ) grades to −100 °C and below. At the hot end, ask for heat-aging data rather than a ceiling.
Grade dependency. Continuous ratings on this page’s grades run from about 175 °C (fluorosilicone) to 200 °C (BISCO foams), 230 °C (kSil GP), and higher for dedicated high-temperature solids; low-temperature limits from −55 °C to below −100 °C.
Cell structure (open, closed, mixed)
What it is. Whether the gas cells in a cellular silicone are isolated (closed), interconnected (open), or a mix. ASTM D1056 defines Type 1 (open) and Type 2 (closed, with a water-absorption limit). [20]
How to use it. Closed cells (sponge) block water and air at low compression and behave like a gas spring. Open cells (MF1 bun, urethane foams) compress with less force, breathe, and recover with lower set, but they absorb liquids and must be skinned, faced, or kept out of wet zones. Cast BISCO foams are mixed; their sheets have no molded skin, so face treatment (PSA, liner, or a laminated film) is part of the sealing design.
Grade dependency. Structural, by manufacturing route; not adjustable by the converter.
Water sealing and water absorption
What it is. Two different things: bulk water absorption of the material (D1056 immersion, percent by weight) and the leak rate of a gasket under a water head at a given compression and width.
How to use it. A 1.5 psi head is roughly the pressure at 1 m immersion (IPX7). In Rogers’ tests, BISCO BF-1000 leaked 47 mL/min at 0.125 in wide and 2 mL/min at 0.5 in wide at that head; HT-800 leaked 11.7 mL/min at only 10% compression. Width and deflection matter more than grade once the material is closed-cell or foam. [5] Map the enclosure rating first (NEMA Type 4/4X ≈ IP66, Type 6/6P ≈ IP67 by NEMA’s own comparison), then set deflection: 40–50% for sponge and foam water seals and 20–30% for solid per NEDC; Rogers uses 30–50% for cellular silicone. [52] [16]
Grade dependency. Absorption 0.2–5% for closed and cast foams; leak rate is a design property, not a material property.
Weathering (outdoor exposure)
What it is. Combined resistance to sunlight, moisture, temperature cycling, and atmospheric ozone. Silicone’s Si–O backbone has no carbon–carbon double bonds to attack, so it weathers with little change in hardness or elongation, which is why it is chosen for outdoor telecom, solar, and transit seals without the carbon-black loading EPDM needs.
Measured by. ASTM G154 (fluorescent UV/condensation) and G155 (xenon arc) accelerated exposure; outdoor racks per ASTM D1171 for ozone. [53]
How to use it. Treat weathering as a pass for unfilled silicone and turn attention to what fails first outdoors: the adhesive bond, the enclosure’s compression set at summer temperature, and water ingress at corners and splices.
UV and ozone resistance
What it is. Resistance to cracking under ultraviolet light and to ozone attack under strain. Ozone cracking is measured in a controlled chamber per ASTM D1149 (pphm ozone, static or dynamic strain). [3]
How to use it. Silicone is one of the few elastomers, with EPDM and FKM, that can be specified next to corona-producing electrical equipment (switchgear, motors, ozone generators, UV sanitizers) without a dedicated ozone test. Nitrile, natural rubber, and neoprene are the ones to avoid there.
Grade dependency. Low; essentially a family property of VMQ and FVMQ.
Chemical and fluid resistance
What it is. Change in volume, hardness, tensile, and elongation after immersion in a fluid at temperature, per ASTM D471 using reference oils (IRM 901/902/903) and fuels. [54]
How to use it. VMQ is good in water, steam, dilute acids and alkalis, alcohols, and most CIP chemistry; poor in hydrocarbon fuels and oils, chlorinated and aromatic solvents, and concentrated acids. Fluorosilicone fixes the fuel and oil case (swell under 5% in IRM 903 versus 26–30% for VMQ in one manufacturer’s data) but not ketones or brake fluid. For anything else, check the rubber chemical compatibility chart and ask for immersion data in your fluid. [6]
Grade dependency. Polymer-dependent (VMQ vs FVMQ); filler can add its own sensitivity (silver-filled grades and salt fog, for example).
Electrical properties (dielectric strength, resistivity, conductivity)
What it is. For insulating grades: dielectric strength (ASTM D149, V/mil, thickness-dependent), volume resistivity (ASTM D257, Ω·cm), dielectric constant and dissipation factor (D150). For conductive grades: volume resistivity (ASTM D991) and shielding effectiveness (MIL-DTL-83528 method, dB). [55]
How to use it. Insulation: convert V/mil at the tested thickness to your thickness with margin, and remember that creepage, clearance, and pollution degree are set by the equipment standard, not the material. Conductive: specify the Type or grade, the resistivity maximum, and the frequency band; verify galvanic compatibility with the flange. Use the dielectric withstand calculator.
Grade dependency. Spans 10¹⁴ Ω·cm (insulating foam) to 0.004 Ω·cm (silver/copper Type A): sixteen orders of magnitude within one polymer family.
Thermal properties (conductivity, impedance)
What it is. Thermal conductivity (W/m·K) is a material property; thermal impedance (°C·in²/W) is what a joint actually pays at a given thickness and pressure, per ASTM D5470. [56]
How to use it. Unfilled silicone foam is an insulator (HT-800 0.076 W/m·K); solid VMQ about 0.2–0.25 W/m·K; filled gap pads 1–5+ W/m·K. For a heat path, compare candidates by D5470 impedance at your clamping pressure and thickness (Sil-Pad TSP 3500 lists 0.57 to 0.20 °C·in²/W from 10 to 200 psi at 0.010 in), not by W/m·K. For a barrier (thermal-runaway, fire), the low conductivity of foam is the feature. [4] [57]
Flammability (UL 94, FAR 25.853, transit FST)
What it is. Behavior in a small-flame test (UL 94: HB, V-2, V-1, V-0, 5V; HBF/HF-1/HF-2 for foams), in the aircraft vertical-burn, heat-release, and smoke tests of FAR 25.853 Appendix F, and in the rail flame-spread and smoke methods (ASTM E162/E662, EN 45545-2). [12] [29]
How to use it. Match the test to the equipment standard (UL 50E/UL 508 enclosures, FAR 25 cabin interiors, NFPA 130 rail), specify the grade and thickness that carries the rating, and keep the test report with the drawing. Silicone chars rather than drips and releases relatively low smoke, which is why V-0 and FST grades exist across foam, sponge, and solid.
Grade dependency. Rating is per grade and thickness; adhesive and liner can change the result on a laminate.
Outgassing (TML, CVCM, WVR)
What it is. Mass lost under vacuum at 125 °C for 24 h (TML), the fraction that condenses on a 25 °C collector (CVCM), and the part that was just water (WVR), per ASTM E595. NASA screening criteria are TML ≤1.0% and CVCM ≤0.10%. [13]
How to use it. Screen every material in the enclosure, including adhesives and liners, against CVCM first; that is the number that fogs optics and contaminates connectors. Most silicone foams pass TML and fail CVCM; specific low-volatile solid grades pass both. For terrestrial optics and sensors, the same logic applies at lower temperatures.
Grade dependency. HT-800 CVCM 0.25%; HT-820 0.63%; H-O low-outgassing sheet ≤0.10%. [4] [30]
Stress relaxation (force retention)
What it is. The decay of sealing force over time at constant deflection. Compression set measures lost thickness after release; stress relaxation measures lost force while still compressed, which is what a bolted or latched gasket experiences. Most of it happens in the first 1–2 hours. [5]
How to use it. Size the initial closure force so that the retained fraction still exceeds the sealing pressure. Rogers’ sealing guide reports silicone foam and PORON® retaining 45–75% of initial force at 60 h versus 15–35% for EPDM and neoprene at 25% compression. [5] This is the property behind silicone’s reputation for long-term sealing.
Questions engineers ask about this topic
Direct answers with the source. The same questions appear in the page’s structured data.
What temperature can silicone rubber withstand?
It depends on the grade, and the continuous rating is the one to design to. BISCO® HT/BF foams list −55 to +200 °C; kSil® GP solids list −60 to 230 °C with 250 °C intermittent; dedicated high-temperature solids publish heat-aging data at 300 °C rather than a ceiling. Standard VMQ stays flexible to about −55 °C, phenyl grades to −100 °C and below. Adhesives and liners are usually the lower limit: acrylic PSA to about 149 °C, silicone PSA to about 232 °C on Rogers’ bulletin. [26]
What is compression set and how much is acceptable for a silicone gasket?
Compression set is the permanent thickness loss after a material is held compressed at temperature and released. For cellular silicone on the ASTM D1056 basis (50% deflection, 100 °C, 22 h), Rogers calls under 5% “excellent for long-term sealing”; cast foams achieve 2–5%, blown sponges 15–20%, and AMS sponge specifications allow 60%. For solids, ASTM D395 at 150 °C/70 h with a limit of 25% or lower is the usual callout (BISCO HT-1200 ≤25%). Compare only on the same method, deflection, temperature, and time. [9] [17]
How do I calculate closure force from CFD?
Multiply the compressive stress at your design deflection (from the grade’s force-deflection curve; the TDS “CFD” is the 25% point) by the gasket footprint area. Rogers’ example: 5 psi × 72 in² = 360 lb. Design cellular silicone at 25–35% deflection, keep gasket width at least equal to thickness, and check the force at the top of the CFD spec range, not the typical. The H-O CFD calculator does the arithmetic. [48] [14]
Can durometer be used to specify silicone foam or sponge?
No. Shore A durometer (ASTM D2240) measures indentation on a solid at least 6 mm thick; on a cellular material it reads the cell walls and skin, not the firmness that decides closure force. Sponge and foam are specified by compression force deflection at 25% (ASTM D1056), sometimes with a Shore OO reference. A drawing that says “silicone, 50 durometer” for a cellular gasket leaves the firmness uncontrolled. [50] [20]
What is the difference between compression set and stress relaxation?
Compression set is thickness that does not come back after the load is removed; stress relaxation is force that decays while the part stays compressed, which is what a bolted or latched gasket actually experiences. Most relaxation happens in the first 1–2 hours. Rogers reports silicone foam and PORON® retaining 45–75% of initial force after 60 h at 25% compression versus 15–35% for EPDM and neoprene. Size the initial closure force so the retained fraction still exceeds the sealing pressure. [5] [9]
How much should a silicone gasket be compressed?
Cellular silicone: 25–35% deflection as the working window (Rogers’ recommended minimum to absorb thickness tolerance, surface variation and stress relaxation); 50–70% is permissible but may crush cells. Sponge and foam water seals are often designed at 40–50% (NEDC). Solid silicone: 10–30%, toward the upper end for water. Keep gasket width at least equal to thickness, preferably 1.5×, and hold the gap tolerance to about ±2 mm on a 10 mm foam gasket. [48] [16] [48]
Is silicone UV and ozone resistant?
Yes, as a family property. The silicon-oxygen backbone has no carbon-carbon double bonds for ozone or UV to attack, so VMQ and FVMQ resist cracking in outdoor and corona-producing electrical environments without the antioxidant packages hydrocarbon rubbers need; ozone exposure per ASTM D1149 is rarely a selection driver. What fails first outdoors is usually the adhesive bond or compression set at summer temperature, not the silicone. [3]
References
Every quantitative claim on this page traces to one of the sources below. Reference numbers are shared across all eight pages of the Silicone Materials guide so a value cited as [4] here is the same source as [4] on any other page. Values change between data-sheet revisions; the revision on file at publication governs.
Show all 39 sources cited on this page tap to expand
ASTM D1149 / D1171
Standard Test Methods for Rubber Deterioration: Cracking in an Ozone Controlled Environment (D1149) and Surface Ozone Cracking Outdoors (D1171). astm.org/d1149 ASTM D1171: store.astm.org/d1171
Rogers BISCO® HT-800 data sheet (Pub. 180-070)
Density 22 pcf; CFD 6–14 psi (9.7 typ.); compression set 2.4% typ.; −55 to +200 °C; ASTM D746 −55 °C; UL 94 V-0/HF-1 file E83967; 75 V/mil; 10¹⁴ Ω·cm; 0.076 W/m·K; TML 0.98% / CVCM 0.25%; AMS 3195; FDA 21 CFR 177.2600 extractives (gray). rogerscorp.com (PDF) · H-O product page
Rogers Technical Sealing Guide (PORON® and BISCO®)
Stress relaxation mostly in first 1–2 h; silicone/PORON retain 45–75% of force at 60 h vs 15–35% for EPDM/neoprene; compression-set comparison at 70 °C and 100 °C (D3574 basis); water leakage vs width and compression at 1.5 psi; NEMA/IP mapping; UL 50E gasket test levels. rogerscorp.com (PDF)
Shin-Etsu silicone rubber performance data
Oil-swell comparison: general silicone +26–30% volume in IRM 903 (150 °C/70 h) vs fluorosilicone under 5%; fluorosilicone in Fuel C about +4%; compression-set and heat-aging ranges by grade. shinetsusilicone-global.com (PDF)
H-O TDS: Extreme High-Temperature Grade Silicone Sheeting
55/60 Shore A; 1,050/1,200 psi; 450%; heat aging 168 h at 300 °C: retained tensile >750 psi, elongation >90%, tear >70 ppi. H-O product page · TDS (PDF)
Rogers: “Everything You Need to Know About Compression Set” (2024)
ASTM D1056 vs D3574 conditions and formulas (2% D1056 ≈ 1% D3574); under 5% “excellent for long-term sealing”; HT-800 about 2%, “rebounds to 99% of original height”; compression set vs stress relaxation. rogerscorp.com
BISCO® RS-700 series sponge data (Rogers via Insul-Fab)
RS-720 17.5 pcf 5–12 psi; RS-750 24 pcf 6–14 psi; RS-770 29 pcf 12–20 psi; compression set 15–20% max (D1056, 100 °C/22 h); −55 to 205 °C; UL 50/50E/508 recognized. insulfab.net (verify against the current Rogers TDS before publication)
H-O TDS: Medical Grade Silicone Sheeting
30–70 Shore A; tensile 1,100–1,350 psi; elongation 600–900%; tear 170–205 ppi (Die B); USP Class VI, European Pharmacopeia, ISO 10993, FDA 21 CFR 177.2600. H-O product page · TDS (PDF)
UL 94, Standard for Tests for Flammability of Plastic Materials
HB, V-2, V-1, V-0, 5VA/5VB and foam classes HBF/HF-1/HF-2; V-0 afterflame ≤10 s per specimen, ≤50 s per set, no flaming drips igniting cotton. ul.com
ASTM E595 and NASA outgassing criteria
125 °C, 24 h, vacuum, 25 °C collector; screening pass TML ≤1.0% and CVCM ≤0.10%. NASA GSFC outgassing database
Rogers: “The Ultimate Guide to Compression Force Deflection” (2024)
CFD per ASTM D1056 at 25%; 25–35% minimum compression recommended; 50–70% permissible but may crush cells; CFD curves at 10/30/50/70%. rogerscorp.com
NEDC: compression rates in rubber gaskets
Solid gaskets 10–30% (air 10–15%, water 20–30%); foam and sponge 30–50% (air 25–35%, water 40–50%). nedc.com
Rogers BISCO® HT-1200 series data sheet (Pub. 180-068)
HT-1240/1250/1260/1270: 40–70 Shore A; compression set ≤25% (ASTM D395, 150 °C/70 h); −68 to 218 °C (−80 to 425 °F); 0.031–0.125 in. rogerscorp.com (PDF)
kSil® GP solid sheet TDS (Silicone Engineering, SE-NEU-V7-2019) and H-O GP50 page
GP30–GP80: tensile 7–10 MPa, elongation 215–525%, tear 16–23 N/mm, compression set 9–25% (ISO 815, 24 h/150 °C) and 10–22% (ASTM D395 B, 22 h/300 °F); −60 to 230 °C (250 °C intermittent); 0.24 W/m·K; 23 kV/mm; 3×10¹⁵ Ω·cm; FDA 21 CFR 177.2600, BfR XV, WRAS, FAR 25.853. TDS (PDF, distributor-hosted) · silicone.co.uk/ksil · H-O GP50 page
SAE AMS 3195 / AMS 3196
AMS 3195 “Silicone Rubber Sponge, Closed Cell, Medium”; AMS 3196 “Silicone Rubber Sponge, Closed Cell, Firm”; compression-set requirement 60% max at 22 h/100 °C per manufacturer conformance pages. sae.org/ams3195 · sae.org/ams3196
ASTM D1056-20 (and D6576)
Standard Specification for Flexible Cellular Materials, Sponge or Expanded Rubber: Types 1/2, Classes A–D, Grades 0–5 by CFD at 25% (under 2, 2–5, 5–9, 9–13, 13–17, 17–25 psi), water-absorption limit for Type 2, suffix tests. ASTM D6576 (silicone sponge, successor to MIL-R-6130) uses the same bands with Super Soft to Firm names. astm.org/d1056
Saint-Gobain Norseal® R10460 sponge TDS (Form 1349)
29 pcf; CFD 10 psi; compression set 5% (D1056); −100 to +500 °F; UL 94 HBF; water absorption under 5%; AMS 3195, MIL-R-6130 Type II, ASTM D6576 Type 2, FDA 21 CFR 177.2600. saint-gobain.com (R10480M page) and the R10460 TDS on file.
Rogers BISCO® pressure-sensitive adhesive options (technical bulletin)
Acrylic PSA: −31 to 149 °C, 75 oz/in peel (20 min dwell), 18-month shelf life, one or two sides. Silicone PSA: −51 to 232 °C, 25 oz/in peel, 0.002 in unsupported, PET liner, 6-month shelf life, one side. PSA nomenclature (A / 2A / S; “5” on cellular grades). tools.rogerscorp.com
14 CFR Part 25, Appendix F (FAR 25.853)
Part I vertical burn (60 s: burn length ≤6 in, flame time ≤15 s; 12 s: ≤8 in); Part IV heat release (peak ≤65 kW/m², total ≤65 kW·min/m²); Part V smoke (Ds ≤200 at 4 min). ecfr.gov
H-O TDS: Low Outgassing Silicone Sheeting
40–70 Shore A; 1,100–1,250 psi; 650–900%; tear 175–200 ppi; TML ≤1.00%, CVCM ≤0.10% (ASTM E595); NASA-STD-6016; FDA 21 CFR 177.2600. H-O product page · TDS (PDF)
Rogers BISCO® HT-6000 series and HT-6240 data sheet (Pub. 180-093)
HT-6240 Transparent: 40 ±5 Shore A; 1,040 psi; 325%; 112 ppi; SG 1.07; 386 V/mil; −55 to +200 °C. HT-6360 Fire-Safe: 60 A; UL 94 V-0; ASTM E162/E662. rogerscorp.com
Rogers BISCO® EC-2130 data sheet (Pub. 180-034)
Nickel-graphite; volume resistivity under 1.00 Ω·cm; SE 105/108/108/103 dB at 100 MHz/600 MHz/1 GHz/10 GHz; 30 ±5 Shore A; compression set 10% max (D395 B, 70 °C/70 h/25%); −62 to +200 °C. rogerscorp.com (PDF)
Henkel Bergquist® Gap Pad® TGP 3000 and TGP 5000 TDS
TGP 3000: 3.0 W/m·K, Shore OO 30, 3,000 Vac, 0.254–3.175 mm, −60 to 200 °C, 3.2 g/cm³, UL 94 V-0. TGP 5000: 5.0 W/m·K, Shore OO 35, 5,000 Vac, 3.6 g/cm³. henkel-adhesives.com (TGP 3000) · TGP 5000
Rogers: “8 Key Considerations for Designing Reliable Seals and Gaskets” (2025)
Closure-force example 5 psi × 72 in² = 360 lb at 25%; width-to-thickness ≥1:1, prefer 1.5×; gap tolerance about ±2 mm on 10 mm foam. rogerscorp.com · see also enclosure seal mechanics
ASTM D395
Standard Test Methods for Rubber Property, Compression Set: Method A constant force, Method B constant deflection (25%). astm.org/d395
ASTM D2240
Standard Test Method for Rubber Property, Durometer Hardness (Types A, D, O, OO, and others). astm.org/d2240
Rogers BISCO® BF-1000 data sheet (Pub. 180-048)
12 pcf; compression set 1.7% typ. (100 °C/22 h/50%); tensile 38 psi; elongation 86%; water absorption 1.4% typ.; UL 94 V-0/HF-1; 0.063–1.000 in; white, gray, black. rogerscorp.com (PDF)
NEMA enclosure types and IEC 60529 comparison
NEMA Type 4/4X meets or exceeds IP66; Type 6/6P meets or exceeds IP67; the table cannot be used to convert IP to NEMA. IPX7 = temporary immersion at 1 m for 30 min per IEC 60529 (IEC 60529). nema.org (PDF)
ASTM G154 / G155 accelerated weathering
G154 fluorescent UV with condensation; G155 xenon arc full spectrum with water spray. astm.org/g154 ASTM G155: store.astm.org/g155
ASTM D471
Standard Test Method for Rubber Property, Effect of Liquids (IRM 901/902/903 reference oils; fuels). astm.org/d471
ASTM D149
Standard Test Method for Dielectric Breakdown Voltage and Dielectric Strength of Solid Electrical Insulating Materials at Commercial Power Frequencies. astm.org/d149
ASTM D5470
Standard Test Method for Thermal Transmission Properties of Thermally Conductive Electrical Insulation Materials (thermal impedance vs thickness and pressure). astm.org/d5470
Henkel Bergquist® Sil-Pad® TSP 3500 TDS
3.5 W/m·K; 90 Shore A; 4,000 Vac; thermal impedance at 0.010 in: 0.57 / 0.43 / 0.33 / 0.25 / 0.20 °C·in²/W at 10 / 25 / 50 / 100 / 200 psi; UL 94 V-0. Henkel TDS (PDF, distributor-hosted)
ASTM D3574
Standard Test Methods for Flexible Cellular Materials, Slab, Bonded, and Molded Urethane Foams (Test C CFD, Test D compression set at 50%/22 h/70 °C). astm.org/d3574
Rogers BISCO® HT-840 data sheet (Pub. 180-321)
27 pcf (family page: 28); CFD 22 psi; compression set 1.8% typical, under 5% specification (D1056, 100 °C/22 h/50%); 0.09 W/m·K; 57 V/mil per current Rogers TDS 180-321; 1/16–1/4 in gray. rogerscorp.com (TDS on file)
Silicone Engineering: expanSil™ GP sponge TDS (SE-NEU-V7-2019)
GP200–GP530: density 200–530 kg/m³; CFD at 25% 28–214 kPa (ASTM D1056); compression set 3.0–5.0% (70 °C/22 h) and 4.3–6.7% (100 °C/22 h) per the TDS test method; −60 to 230 °C. Extrusion grades, cited for the closed-cell sponge compression-set benchmark. TDS (PDF, distributor-hosted) · silicone.co.uk/expansil
Saint-Gobain Norseal® silicone rubber solutions brochure
Sponge, foam, and solid grade table including R10490 fluorosilicone sponge (35 pcf, 15 psi, compression set 25%, −80 to +400 °F). Where the brochure and a grade TDS disagree, the TDS governs. saint-gobain.com (PDF)
Rogers PORON® 4701-50 data sheet
15/20/30 pcf; CFD 10–39 psi (D3574 C); compression set ≤10% (D3574 D, 70 °C); continuous 90 °C, intermittent 121 °C; 0.012–0.5 in. rogerscorp.com
BISCO® 7xxx series sponge TDS (Rogers, hosted on H-O product pages)
7130 Soft FR: 31 pcf, CFD 2–7 psi at 25%, C-set 35% (22 h at 212 °F), −67 to 400 °F, UL 94 HBF, BMS 1-60 Type 1 Grade A and DMS-1980 Grade 1 per the Rogers TDS. 7304 Medium: 35 pcf, 6–14 psi, C-set 20%, −67 to 450 °F, BMS 1-23, red. 7330 Firm FR: 35 pcf, 7–14 psi, C-set 35%, −67 to 450 °F, BMS 1-60 Type 1 Grade B, DMS-1980 Grade 2; 0.313–1.00 in. 7430 Firm FR: 35 pcf, 14–22 psi, C-set 35%, −67 to 400 °F, BMS 1-60 Type 1 Grade C; 0.188–0.500 in. Water absorption under 5%; UV and ozone resistant. 7130 · 7304 · 7330 · 7430 (Rogers TDS PDFs on each page; confirm current revision with Rogers before publication)
Need help selecting a silicone?
Send H-O your drawing, operating temperature, environment, compression requirements, regulatory requirements, adhesive needs, and expected quantity. Our team reviews the application against current manufacturer data and helps identify appropriate material constructions for prototyping and production. We typically respond within one business day.
See also: the rest of the Silicone Materials guide
The guide is one hub and seven topic pages that share one set of sources and one set of numbers.