Silicone Foam vs Silicone Sponge vs Solid Silicone: Structure, Compression and Selection
The three forms of silicone share a chemistry and almost nothing else that matters to a gasket. This page explains how solid sheet, blown closed-cell sponge, and cast cellular foam are made, how each is rated, how each compresses, seals, and recovers, and which one to specify for a given joint.
Part of the Silicone Materials guide. Start at the hub page for the forms, the selection matrix and the material families; this page goes deep on one topic.
Solid silicone is rated by durometer and needs high closure force; closed-cell sponge is rated by CFD, carries a molded skin, and sets 15–20% on the D1056 basis; cast foam is rated by CFD, seals at the lowest force, and sets 2–5%. Specify the grade or specification, never the word “foam” or “sponge,” and state compression set with its test basis. H-O converts all three from sheet and roll stock into die-cut, kiss-cut and laminated parts. Skip to the quote form →

Silicone sponge is a high-consistency silicone gum expanded with a blowing agent into closed, non-interconnecting cells under a molded skin. Silicone foam (BISCO® HT/BF type) is a liquid two-part silicone cast onto a carrier and addition-cured, with an irregular, partly open cell structure and no molded skin. Solid silicone is non-cellular sheet rated by Shore A durometer. Sponge and foam are both rated by compression force deflection at 25% (ASTM D1056), but cast foam recovers to about 98% of its thickness after 22 h at 100 °C while blown sponge typically recovers to 80–85%.
Property values are quoted from the source manufacturer TDS or the cited standard, not from H-O testing. H-O converts sheet and roll silicone; ratings belong to the specific grade and a finished assembly earns its own rating at the system level.
- Low closure force, thin flange: silicone foam
- Firmer seal with a skin, mil/AMS callout: closed-cell sponge
- Bolted flange, washer, pressure: solid sheet
-
1Send drawingUpload a DXF, STEP, or PDF, or describe the gasket, pad, or insulator and its environment. A sample part works too.
-
2Material reviewEngineering checks the candidate grade against the manufacturer TDS: closure force, compression set, service temperature, fluid exposure, flame or regulatory requirement, and adhesive compatibility.
-
3Prototype24-hour prototypes on in-house materials; otherwise samples typically ship in 3–5 business days for common die-cut configurations on materials we commonly convert. Made-to-order; MOQ varies by material and part.
-
4ProductionStandard production runs ship about 2 weeks after drawing approval, including kiss-cut-on-liner and laminated configurations. Expedited service available. Ongoing parts run with lot traceability and TDS records.
Silicone foam vs silicone sponge vs solid silicone
The three forms share a chemistry and almost nothing else that matters to a gasket. Solid silicone is a non-cellular rubber rated by durometer. Silicone sponge is a high-consistency rubber expanded with a blowing agent into closed cells under a molded skin. Silicone foam is a liquid two-part system that is cast and cured, with the cure reaction itself generating the gas that expands the matrix. The manufacturing route sets the cell structure, the cell structure sets the compression behavior, and the compression behavior sets closure force, sealing pressure, and long-term recovery.
“Foam” and “sponge” are not interchangeable engineering terms. Some manufacturers use them loosely, and Rogers itself calls RS-700 series “sponge” and HT-800 series “cellular silicone” while some distributors call both “foam.” On a drawing, call out the grade or the specification (AMS 3195, ASTM D1056 2D2, ASTM D6576 Soft-Medium) rather than the word. The two materials differ by a factor of about 5–10 in compression set on the same test basis. [9] [10]
Engineering comparison
| Attribute | Solid silicone | Silicone sponge | Silicone foam |
|---|---|---|---|
| Structure | Non-cellular. Reinforced with fumed or precipitated silica; optionally fabric or fiberglass. | Closed, non-interconnecting cells with a molded skin on both faces (sheet) or all faces (extrusion). Type 2 under ASTM D1056. | Irregular cellular structure, predominantly closed but with some open cells; no molded skin on cast sheet. Rogers does not label HT/BF foams “open” or “closed.” |
| How it is measured | Shore A durometer (ASTM D2240); tensile, elongation (D412); tear (D624); compression set (D395). | Compression force deflection at 25% (D1056); density; compression set (D1056 Test D); water absorption; firmness bands per ASTM D6576 or AMS 3195/3196. | Same cellular methods as sponge. Rogers publishes force-vs-deflection data across the deflection range for BISCO grades, not only the 25% point. [14] |
| Typical firmness range | 10–90 Shore A across the catalog; 30–70 A most common for gaskets. | About 2–25 psi at 25% (ASTM D6576 Super Soft through Firm). BISCO RS-700: 5–20 psi; kSil® KSV001–006: 2.8–9 psi and up. [10] [15] | Under 2 psi typical (BF-2000, 2.5 psi max) to about 21 psi typical (HT-840, 16–26 psi specification) at 25%. [8] |
| Compression behavior | Nearly incompressible in bulk; it deforms by displacement. Needs 10–30% deflection and a high force per unit area; a groove or flange must give it room to move. | Cells resist collapse until the skin and walls buckle; force rises steeply past about 40–50% deflection. Design deflection 30–50% is common (NEDC); 30–40% is the conservative end. [16] | Lowest force for a given deflection; Rogers recommends 25–35% minimum deflection and warns that 50–70% may crush cells. [14] |
| Compression set (recovery) | BISCO HT-1200 solids: ≤25% (D395, 150 °C/70 h). kSil GP50: 16% (D395 B, 22 h/300 °F). Peroxide-cured solids without post-cure set more. [17] [18] | Typically 15–20% (D1056, 100 °C/22 h/50%) for RS-700 class; AMS 3195/3196 allow up to 60%. Set is the main long-term risk. [10] [19] | About 2–5% (HT-800 2.4% typ., BF-1000 1.7% typ.) on the same D1056 basis. Rogers calls under 5% “excellent for long-term sealing.” [9] |
| Sealing behavior | Best for high contact pressure: bolted flanges, fluid pressure, high-vacuum. Poor at bridging uneven gaps without high force. | Closed cells do not wick; smooth skin seals against dust and water at moderate force. Good NEMA / IP gasket where flanges are stiff enough to develop 30%+ deflection. | Best seal per pound of closure force; water sealing depends on width and deflection (HT-800 leaked 11.7 mL/min at only 10% compression at a 1.5 psi head in Rogers’ test). Surface cells can hold water, so skin, liner, or PSA face matters. [5] |
| Mechanical performance | Highest tensile, tear, and abrasion of the three; handles bolt holes, thin webs, and repeated installation. | Moderate; skin resists surface tearing; thin die-cut webs are workable above about 1/16 in. | Lowest tensile (tens of psi). Fragile webs and narrow lands need a carrier or a wider design; IF-200 adds a fiberglass support layer for this reason. |
| Water absorption | Negligible. | Under 1–5% typical (closed cell, D1056 requirement for Type 2). [20] | HT-800 0.5% typ., BF-1000 1.4% typ. on the Rogers basis; foam faces can still trap surface water. [4] |
| Typical thickness | 0.010–0.500 in (thin-gauge to 0.005 in in some medical/reinforced grades) | 0.031–0.500 in sheet; sponge up to 45 mm from some mills | 0.031–0.500 in sheet (MF1 bun to 8 in) [8] |
| Typical applications | Flange gaskets, washers, spacers, electrical insulators, high-pressure seals, food-line seals, vacuum-membrane blanks, thermal and EMI pads (filled) | Enclosure door gaskets, HVAC and switchgear seals, aircraft interior seals to AMS 3195/3196, food-processing sponge seals, flame-rated transit gaskets | Low-force enclosure and lid seals, EV battery cushioning pads, vibration isolation, thermal-runaway barrier layers, aircraft interior cushioning, thin conformable environmental seals |
| Reason to choose it | Strength, pressure capability, thin gauges, widest specialty formulation range | Firmer sealing with a skin, familiar mil/AMS callouts, lower cost per sheet than cast foam in many grades | Lowest closure force and lowest compression set of any silicone form; best at thin flanges, plastic housings, and long-term seals |
| Primary limitation | Needs high closure force and a controlled gap; will not bridge warped flanges | Higher compression set than foam; firmness bands are wide; blowing agents and peroxide by-products limit some regulatory uses | Low tear strength, higher price per sheet, and surface cells that need a liner, skin, or PSA face for some sealing and cleaning duties |
How to read the firmness bands. ASTM D1056 grades 0–5 correspond to CFD at 25% of under 2, 2–5, 5–9, 9–13, 13–17, and 17–25 psi; ASTM D6576 uses the same bands with the names Super Soft, Soft, Soft-Medium, Medium, Medium-Firm, and Firm. Silicone sponge is usually called out as Type 2 (closed cell) Class D (extreme temperature), so a “2D2” sponge is a 5–9 psi closed-cell silicone, and AMS 3195 is the Medium closed-cell sponge specification while AMS 3196 is Firm. [20] [19]
Solid silicone, silicone sponge, and silicone foam as converted materials
Each form below is described as a converter sees it: the sheet or roll product that arrives from the silicone manufacturer, the grades that exist, and what changes when it is die-cut, laminated, and installed. H-O does not compound, calender, cast, mold, or extrude silicone; those processes belong to the material manufacturer and are described only so the resulting properties make sense.
Solid silicone rubber sheet
What it is. Non-cellular silicone made from a high-consistency rubber (HCR) gum compounded with reinforcing silica, pigments, and a cure package, then calendered into continuous sheet or compression-molded into sheets and cured. Calendered sheet is the standard converting stock; molded sheet is used where a tighter thickness tolerance or a specific surface finish is required. Some thin-gauge medical and reinforced products are cast or coated onto fabric or film.
Durometer is the primary callout, and it is not a seal rating. A 30 Shore A sheet conforms to flange imperfections at lower force; a 70 Shore A sheet resists extrusion under pressure and holds a bolt-hole pattern. Tensile, elongation, and tear move with durometer but not linearly. On H-O’s commercial-grade sheets, 50 Shore A FDA white silicone lists 950 psi tensile, 600% elongation, and 105 ppi tear (ASTM D412/D624), while the USP Class VI / ISO 10993 medical-grade family runs 1,100–1,350 psi and 170–205 ppi across 30–70 Shore A. [21] [11] The durometer scale chart compares Shore A, OO, and D.
Grade families you will meet. Commercial grades (typically red or black, 30–90 A) for general gasketing; FDA-compliant white and translucent grades; military and aerospace grades called out to A-A-59588 (the 2001 successor to ZZ-R-765) by Class and Grade, and to AMS 3301–3305 by durometer; high-strength and high-tear grades (A-A-59588 Class 3) where bolt holes or repeated assembly tear ordinary sheet; translucent grades, which are simply unpigmented and are useful where visual inspection of a seal or fluid path matters; reinforced sheet with a woven fiberglass or polyester ply for dimensional stability; and thin-gauge sheet down to 0.005 in in some grades (H-O’s low-outgassing sheet lists 0.005 in minimum) for insulators and diaphragms. [30] [22]
Cure and post-cure. Most commercial solid sheet is peroxide-cured; medical and many FDA grades are platinum-cured. Peroxide-cured sheet is normally post-cured by the manufacturer to drive off cure by-products and stabilize compression set; a sheet that is not post-cured will harden and lose elongation in service. See cure systems.
Converting notes. Solid sheet die-cuts cleanly at all common durometers; thick, soft sheet (over 1/8 in, under 40 A) can distort under a steel-rule die and is a candidate for waterjet or CNC knife cutting. Solid silicone is the form most often laminated with a silicone PSA or a differential (silicone/acrylic) tape. Grades on this site: Solid Silicone Rubber category.
Silicone sponge (closed-cell expanded silicone)
What it is. A silicone gum compound containing a chemical blowing agent is calendered or molded and then heated; the blowing agent decomposes to gas while the peroxide cross-links the rubber, and the result is a network of closed, non-interconnecting cells. Sheet sponge carries a smooth molded skin on both faces. Because the cells are closed, water absorption is low (ASTM D1056 requires under 5% for Type 2 above 10 pcf) and the material does not wick. [20]
Firmness and compression. Sponge is bought by firmness, not durometer. Manufacturers express it as CFD at 25% deflection with a band (for example, BISCO RS-720 5–12 psi, RS-770 12–20 psi) and Shore OO is sometimes given for reference. kSil® KSV001 V-0 sponge lists 2.8 psi at 25% and 10 pcf; KSV004 lists 9.0 psi and 24.3 pcf, which shows how much density and firmness track each other within one family. [10] [15] Design deflection of 30–50% is the common target for sponge gaskets per NEDC, with 30–40% the conservative end; beyond about 50% the closed cells begin to collapse and force rises steeply. [16]
The compression-set caveat. Blown sponge sets more than cast foam. RS-700 sponge lists 15–20% maximum compression set (D1056, 100 °C/22 h) against the 2–5% typical of HT-800 foam, and the AMS 3195/3196 specifications permit as much as 60%. A sponge gasket that meets AMS 3195 can still lose most of its sealing force in a hot, permanently compressed joint; specify the compression-set value, not only the specification. [10] [19]
Grade families. Flame-retardant sponge (BISCO RS-800/820/840/870; aerospace-specification BISCO 7130/7304/7330/7430, covered below; kSil® V-0 KSV001–006 with UL 94 V-0 and EN 45545-2 data) for switchgear, transit, and aircraft interiors; FDA-compliant sponge (white or red grades; Saint-Gobain Norseal® R10460 lists FDA 21 CFR 177.2600, AMS 3195, and ASTM D6576 on one TDS); fluorosilicone sponge (Norseal R10490, 35 pcf, 15 psi, −80 to +400 °F) for fuel and oil zones; and sound-barrier sponge (BISCO A2). [23] [24]
Aerospace-specification sponge: BISCO® 7xxx series. Rogers’ 7xxx grades are the sponge line qualified to the airframe material specifications rather than to a UL file: 7130, 7330 and 7430 meet Boeing BMS 1-60 Type 1 (Grades C, B and C respectively), 7330 also meets Douglas DMS-1980 Grade 2, and 7304 meets BMS 1-23. They are denser than the RS series (31–35 pcf) and come in thick gauges up to 1.00 in, which is why they turn up in cabin-door, airframe-access and galley seals where the drawing names the spec, not the brand. Note the trade-off: the FR grades list 35% compression set at 212 °F, so they hold a flame and specification requirement rather than a long-term recovery requirement; use foam where recovery governs. [68]
| Grade | Density | CFD at 25% | C-set (22 h, 212 °F) | Service range | Specification | Gauge · color |
|---|---|---|---|---|---|---|
| 7130 Soft FR | 31 pcf | 2–7 psi | 35% | −67 to 400 °F | BMS 1-60 Type 1 Gr. A; DMS-1980 Gr. 1; UL 94 HBF | per catalog · gray |
| 7304 Medium | 35 pcf | 6–14 psi | 20% | −67 to 450 °F | BMS 1-23 | per catalog · red |
| 7330 Firm FR | 35 pcf | 7–14 psi | 35% | −67 to 450 °F | BMS 1-60 Type 1 Gr. B; DMS-1980 Gr. 2 | 0.313–1.00 in · gray |
| 7430 Firm FR | 35 pcf | 14–22 psi | 35% | −67 to 400 °F | BMS 1-60 Type 1 Gr. C | 0.188–0.500 in · gray |
Values from the Rogers TDS hosted on the H-O product pages for 7130, 7304, 7330 and 7430. [68] Specification conformance is a property of the material lot; ask for the certificate of conformance with the order.
Converting notes. The skin gives sponge a clean die-cut edge and a good PSA bonding face. Kiss-cutting on a liner is routine. Because the skin is where the seal happens, avoid designs that rely on a cut edge as the sealing face. Grades on this site: BISCO RS sponge, kSil® V-0 sponge, fluorosilicone sponge.
Silicone foam (cast cellular silicone)
What it is. A two-part liquid silicone system is metered, mixed, cast onto a carrier, and cured by platinum-catalyzed addition. The cure reaction releases hydrogen gas that expands the material as it gels, so the cells form during cure rather than from a separate blowing agent. The result is a lower-density material with an irregular cell structure, no molded skin, and a notably low compression set. Rogers’ data sheets describe the HT/BF family as “cellular silicone” and reports compression set of about 2% for HT-800, which it characterizes as “rebounding to 99% of original height.” [9]
The BISCO® firmness ladder. All HT/BF grades share the same base chemistry and −55 to +200 °C rating, UL 94 V-0 and HF-1 recognition under file E83967, and FMVSS 302 results; they differ in density and CFD: BF-2000 about 11 pcf and 1.5 psi typical; BF-1000 12 pcf; HT-870 15 pcf and 2–7 psi; HT-800 22 pcf and 6–14 psi (9.7 typical); HT-820 24 pcf and 12–20 psi; HT-840 about 27–28 pcf and 22 psi. HT-800 carries AMS 3195 and HT-820 AMS 3196; gray HT-800 has been evaluated against the FDA 21 CFR 177.2600 extractives limits. [8] [4] [25]
Modified and higher-density constructions. Beyond the sheet foams, the family includes MF1 open-cell bun foam (5–7 pcf, cast up to 8 in thick, used for rail seating and thermal-runaway barriers), IF-200 tear-resistant foam with a bonded fiberglass support layer, RF-120 heat shield (BF-1000 foam cast on aluminized fabric), FPC fire-barrier foam, and medical MS-series foams and buns. These are engineered constructions, not new chemistries. [8]
Why engineers choose foam. Closure force. A plastic enclosure lid, a thin sheet-metal door, or a battery-module frame cannot develop the force a solid gasket needs; a 2–7 psi foam seals at a fraction of that force and keeps most of it after thermal cycling. The trade is mechanical fragility (tensile in the tens of psi) and price per sheet.
Converting notes. Foam is supplied on a liner or with PSA on one or two faces (Rogers nomenclature adds a “5” to the grade for PSA-backed material, e.g. HT-805). Kiss-cut parts on liner are the standard delivery. Narrow lands under about 1/8 in in soft grades need care; wider gaskets also seal better (in Rogers’ sealing guide, BF-1000 leakage at a 1.5 psi head fell from 47 mL/min at 0.125 in wide to about 2 mL/min at 0.5 in). [5] Grades on this site: BISCO HT / BF series, MF1 bun, RF-120 / IF-200 / FPC.
Questions engineers ask about this topic
Direct answers with the source. The same questions appear in the page’s structured data.
What is the difference between silicone foam and silicone sponge?
Silicone sponge is a high-consistency silicone gum expanded with a chemical blowing agent into closed, non-interconnecting cells under a molded skin, usually peroxide-cured. Silicone foam (BISCO® HT/BF type) is a liquid two-part silicone cast onto a carrier and addition-cured, with an irregular, partly open cell structure and no molded skin. Both are rated by compression force deflection (ASTM D1056), but their compression set differs by roughly an order of magnitude on the same basis: about 2–5% for cast foam versus 15–20% typical for blown sponge, with AMS 3195/3196 permitting up to 60%. Specify the grade or specification, not the word. [9] [10]
Silicone sponge vs solid silicone: which one for a gasket?
By closure force and pressure. Solid silicone is nearly incompressible in bulk and needs a high force per unit area and a controlled gap; it is the choice for bolted flanges, fluid pressure, washers, and thin insulators. Sponge compresses at 2–25 psi (25% deflection) and bridges uneven flanges at moderate force with a skin that seals against dust and water; it is the choice for enclosure doors and panels. If the joint cannot supply even that force, use foam. Design deflection: solid 10–30%, sponge and foam 30–50% (NEDC). [16]
What is BISCO® 7xxx silicone sponge, and when do I specify it instead of RS or kSil® V-0 sponge?
The 7xxx series (7130 Soft FR, 7304 Medium, 7330 Firm FR, 7430 Firm FR) is Rogers’ closed-cell silicone sponge qualified to airframe material specifications: BMS 1-60 Type 1 for the FR grades, BMS 1-23 for 7304, and DMS-1980 for 7330. Specify it when the drawing or the customer’s approved-materials list names one of those specifications, or when you need thick sponge (7330 runs to 1.00 in). For a switchgear or HVAC door seal without an airframe callout, RS-800 series or kSil® V-0 sponge usually gives the same closed-cell seal at lower density; where long-term recovery matters more than the spec, cast foam (2–5% compression set) beats any blown sponge. [68]
What is the difference between closed-cell and open-cell silicone?
Closed-cell silicone (sponge, ASTM D1056 Type 2) has gas cells that do not connect, so it blocks water and air at low compression and must show under 5% water absorption above 10 pcf. Open-cell silicone (MF1 bun, ASTM D1056 Type 1) has interconnected cells, compresses with less force and breathes, but absorbs liquid and needs a skin or facing in wet zones. Cast BISCO® HT/BF foams are mixed: predominantly closed with some open cells and no molded skin, so face treatment (liner, PSA, film) is part of the sealing design. [20] [8]
Can I substitute silicone sponge for silicone foam on a drawing?
Only if the drawing controls compression set and the joint can tolerate the difference. A sponge and a foam with the same CFD at 25% can differ by an order of magnitude in compression set on the same test basis (15–20% for blown sponge vs 2–5% for cast foam at 100 °C/22 h/50%), and the sponge’s molded skin changes how it seals and bonds. Substitution in the other direction (foam for sponge) usually costs more per sheet and loses the skin. Call out the grade or specification and the compression-set limit; then the substitution question answers itself. [9] [10]
What thicknesses do silicone foam, sponge and solid sheet come in?
BISCO® HT/BF foams run 0.031–0.500 in, BF-1000 to 1.000 in, and MF1 bun to 8 in. Sponge sheet typically runs 0.031–0.500 in, with some mills to 45 mm. Solid sheet runs 0.010–0.500 in, with thin-gauge medical and reinforced grades to about 0.005 in. Cellular silicone thickness tolerance is typically about ±10% or a stated band; solid sheet is tighter. Availability is grade-specific, so confirm the gauge on the TDS before fixing a gap. [8] [42]
What do AMS 3195 and AMS 3196 mean for silicone sponge?
They are SAE aerospace material specifications for closed-cell silicone sponge: AMS 3195 is the Medium firmness grade and AMS 3196 is the Firm grade. Rogers maps BISCO HT-800 to AMS 3195 and HT-820 to AMS 3196. Both specifications permit compression set up to 60% (22 h at 100 °C), far looser than the 2–5% cast foams achieve, so “meets AMS 3195” by itself does not guarantee low set; specify the value as well as the specification. [19] [4]
References
Every quantitative claim on this page traces to one of the sources below. Reference numbers are shared across all eight pages of the Silicone Materials guide so a value cited as [4] here is the same source as [4] on any other page. Values change between data-sheet revisions; the revision on file at publication governs.
Show all 21 sources cited on this page tap to expand
Rogers BISCO® HT-800 data sheet (Pub. 180-070)
Density 22 pcf; CFD 6–14 psi (9.7 typ.); compression set 2.4% typ.; −55 to +200 °C; ASTM D746 −55 °C; UL 94 V-0/HF-1 file E83967; 75 V/mil; 10¹⁴ Ω·cm; 0.076 W/m·K; TML 0.98% / CVCM 0.25%; AMS 3195; FDA 21 CFR 177.2600 extractives (gray). rogerscorp.com (PDF) · H-O product page
Rogers Technical Sealing Guide (PORON® and BISCO®)
Stress relaxation mostly in first 1–2 h; silicone/PORON retain 45–75% of force at 60 h vs 15–35% for EPDM/neoprene; compression-set comparison at 70 °C and 100 °C (D3574 basis); water leakage vs width and compression at 1.5 psi; NEMA/IP mapping; UL 50E gasket test levels. rogerscorp.com (PDF)
Rogers BISCO® silicones family overview
Grade ladder (BF-2000 10–11 pcf, BF-1000 12 pcf, HT-870 15 pcf 2–7 psi, HT-800 22 pcf, HT-820 24 pcf, HT-840 28 pcf), MF1 bun to 8 in, IF-200, RF-120 (BF-1000 foam on aluminized fabric), FPC, RS-700 sponge, HT-1200 and HT-6000 solids, EC-2130 / EC2265, MS medical series. rogerscorp.com
Rogers: “Everything You Need to Know About Compression Set” (2024)
ASTM D1056 vs D3574 conditions and formulas (2% D1056 ≈ 1% D3574); under 5% “excellent for long-term sealing”; HT-800 about 2%, “rebounds to 99% of original height”; compression set vs stress relaxation. rogerscorp.com
BISCO® RS-700 series sponge data (Rogers via Insul-Fab)
RS-720 17.5 pcf 5–12 psi; RS-750 24 pcf 6–14 psi; RS-770 29 pcf 12–20 psi; compression set 15–20% max (D1056, 100 °C/22 h); −55 to 205 °C; UL 50/50E/508 recognized. insulfab.net (verify against the current Rogers TDS before publication)
H-O TDS: Medical Grade Silicone Sheeting
30–70 Shore A; tensile 1,100–1,350 psi; elongation 600–900%; tear 170–205 ppi (Die B); USP Class VI, European Pharmacopeia, ISO 10993, FDA 21 CFR 177.2600. H-O product page · TDS (PDF)
Rogers: “The Ultimate Guide to Compression Force Deflection” (2024)
CFD per ASTM D1056 at 25%; 25–35% minimum compression recommended; 50–70% permissible but may crush cells; CFD curves at 10/30/50/70%. rogerscorp.com
H-O product pages: kSil® V-0 KSV001 and KSV004 sponge
KSV001 V-0 Super Soft: 10.0 pcf, 2.8 psi at 25%, UL 94 V-0, −76 to 446 °F. KSV004 Medium: 24.3 pcf, 9.0 psi at 25%. KSV001 · KSV004 · manufacturer: silicone.co.uk
NEDC: compression rates in rubber gaskets
Solid gaskets 10–30% (air 10–15%, water 20–30%); foam and sponge 30–50% (air 25–35%, water 40–50%). nedc.com
Rogers BISCO® HT-1200 series data sheet (Pub. 180-068)
HT-1240/1250/1260/1270: 40–70 Shore A; compression set ≤25% (ASTM D395, 150 °C/70 h); −68 to 218 °C (−80 to 425 °F); 0.031–0.125 in. rogerscorp.com (PDF)
kSil® GP solid sheet TDS (Silicone Engineering, SE-NEU-V7-2019) and H-O GP50 page
GP30–GP80: tensile 7–10 MPa, elongation 215–525%, tear 16–23 N/mm, compression set 9–25% (ISO 815, 24 h/150 °C) and 10–22% (ASTM D395 B, 22 h/300 °F); −60 to 230 °C (250 °C intermittent); 0.24 W/m·K; 23 kV/mm; 3×10¹⁵ Ω·cm; FDA 21 CFR 177.2600, BfR XV, WRAS, FAR 25.853. TDS (PDF, distributor-hosted) · silicone.co.uk/ksil · H-O GP50 page
SAE AMS 3195 / AMS 3196
AMS 3195 “Silicone Rubber Sponge, Closed Cell, Medium”; AMS 3196 “Silicone Rubber Sponge, Closed Cell, Firm”; compression-set requirement 60% max at 22 h/100 °C per manufacturer conformance pages. sae.org/ams3195 · sae.org/ams3196
ASTM D1056-20 (and D6576)
Standard Specification for Flexible Cellular Materials, Sponge or Expanded Rubber: Types 1/2, Classes A–D, Grades 0–5 by CFD at 25% (under 2, 2–5, 5–9, 9–13, 13–17, 17–25 psi), water-absorption limit for Type 2, suffix tests. ASTM D6576 (silicone sponge, successor to MIL-R-6130) uses the same bands with Super Soft to Firm names. astm.org/d1056
H-O TDS: 50 Durometer FDA Grade Solid Silicone
SG 1.33; 50 ±5 Shore A; 950 psi; 600%; tear 105 ppi; −80 to 450 °F; FDA 21 CFR 177.2600; 1/32–1/2 in white. H-O product page
SSP: AMS silicone specifications map and SSP352
AMS 3301 (40 A), 3302 (50), 3303 (60), 3304 (70), 3305 (80), 3325 (fluorosilicone 60), 3332 (extreme low temperature 20); SSP352 (AMS 3303) 60 A, 1,000 psi, 350%, 75 ppi, peroxide cure. sspinc.com/ams-silicones · sspinc.com/products/ssp352
Saint-Gobain Norseal® R10460 sponge TDS (Form 1349)
29 pcf; CFD 10 psi; compression set 5% (D1056); −100 to +500 °F; UL 94 HBF; water absorption under 5%; AMS 3195, MIL-R-6130 Type II, ASTM D6576 Type 2, FDA 21 CFR 177.2600. saint-gobain.com (R10480M page) and the R10460 TDS on file.
H-O product page: Norseal® R10490 fluorosilicone sponge
35 pcf; CFD 15 psi; −80 to 400 °F; AMS 3323, MIL-R-6130; 0.031–0.125 in blue. H-O product page · TDS (PDF)
Rogers BISCO® HT-820 data sheet (Pub. 180-071)
24 pcf; CFD 12–20 psi (15.3 typ.); compression set under 5%; 0.09 W/m·K; 66 V/mil; TML 2.11% / CVCM 0.63%; AMS 3196; 0.031–0.250 in gray. rogerscorp.com
H-O TDS: Low Outgassing Silicone Sheeting
40–70 Shore A; 1,100–1,250 psi; 650–900%; tear 175–200 ppi; TML ≤1.00%, CVCM ≤0.10% (ASTM E595); NASA-STD-6016; FDA 21 CFR 177.2600. H-O product page · TDS (PDF)
Silicone Engineering: kSil® sheeting and kSil® VAC membranes
kSil solid 30–80 Shore A, 0.3–20 mm, to 1,800 mm wide; sponge 150–600 kg/m³, 2–45 mm, closed cell; −60 to 230 °C; kSil VAC elongation 780–900%, to 4 mm, translucent. Current family list: kSil, kSil VAC, kSil V-0, metectSil, neutraSil, expanSil, suraSil. silicone.co.uk/ksil · kSil VAC · our materials
BISCO® 7xxx series sponge TDS (Rogers, hosted on H-O product pages)
7130 Soft FR: 31 pcf, CFD 2–7 psi at 25%, C-set 35% (22 h at 212 °F), −67 to 400 °F, UL 94 HBF, BMS 1-60 Type 1 Grade A and DMS-1980 Grade 1 per the Rogers TDS. 7304 Medium: 35 pcf, 6–14 psi, C-set 20%, −67 to 450 °F, BMS 1-23, red. 7330 Firm FR: 35 pcf, 7–14 psi, C-set 35%, −67 to 450 °F, BMS 1-60 Type 1 Grade B, DMS-1980 Grade 2; 0.313–1.00 in. 7430 Firm FR: 35 pcf, 14–22 psi, C-set 35%, −67 to 400 °F, BMS 1-60 Type 1 Grade C; 0.188–0.500 in. Water absorption under 5%; UV and ozone resistant. 7130 · 7304 · 7330 · 7430 (Rogers TDS PDFs on each page; confirm current revision with Rogers before publication)
Need help selecting a silicone?
Send H-O your drawing, operating temperature, environment, compression requirements, regulatory requirements, adhesive needs, and expected quantity. Our team reviews the application against current manufacturer data and helps identify appropriate material constructions for prototyping and production. We typically respond within one business day.
See also: the rest of the Silicone Materials guide